Edge Fracture in Mixed Microstructure Steels

2018-12-05 13:26:00
LUQIMENG
Original
2876

Presentation Outline

? Edge Fracture – Background

? Past Case Studies

? Material Evaluations on Production & Trial Material

? Edge quality effects

? Hole expansion testing on current and new grades of AHSS

? Nano-indentation and microstructure

? Concluding Remarks


Edge Fracture – Background

? Fracture initiating at a trimmed edge, typically not predicted by an FLC

? A local formability phenomena: aninter-relationship between steel microstructure, damage during trimming,  and subsequent edge-stretch during forming.

? AHSS more susceptible than single phase materials (Low Carbon, HSLAs)


Edge Fracture – Background

? Edge fractures typically occur in the highest edge strain area in the presence of a rough trimmed edge.

?Typically during drawing or from a stretch flange after a rough die trim.


Edge Fracture Case Studies

? Edge fracture instances are not isolated to particular steel suppliers, grades of AHSS, gauge, or coating.

? Case study subset selected to show common root causes and resolutions.



Front Compartment Rail – CR780T / 420Y (DP).

? This design is frequently used for double attached left / right compartment rails (material utilization)

? Significant edge stretch condition during the draw in the ‘horse collar’ area

? Also, thin bypass condition between common trim lines (difficult to support) affected trim quality.


Rear Rail CR590T / 340YDP

? Intermittent edge fracture predominantly on one hand of part.

?Size and exact location of fractures were variable run-to-run.


Rear Rail CR590T / 340YDP

? LH vs. RH trim conditions made more robust.

? Trim steel insert maintenance required (sharpening).

Potential Sources of Poor Trim Quality

? Poor Nesting (Trimming in Air)

? Die Breathing and Flexing

? Die Guidance

? Improper Clearance

?Typically too tight

?13-15% recommended for most AHSS

? Sharpness of Trim Steels

Part with Flanged Hole – DP980T / 550Y

? Part hole expansion is 13%

? Material capability is 12-15%

? Other material properties within specification

? Hole Expansion (recently added to qualification approval process in May 2014)

? Design not robust for material capability

? Changed material to high yield ratio CR980T / 700Y-MP-LCE

? (HER ~ 30%)

? No issues-to-date


Try-out vs. Production Blanks

? Laser cut blanks in try-out material are not a good indicator of potential edge fractures in production with die struck blanks.

? Stamping plants are concerned about receiving dies for secondary try-out when the dies have not stamped die struck blanks in primary try-out.

? Timing of production-intended blanks needs to ensure that delivery occurs before dies are shipped to home line.


Hole Expansion Testing

? Variability of hole expansion testing exists due to variation in microstructure within a material, the quality of the sheared hole, and specific testing equipment site-to-site.

? A tool for qualification of material and general understanding of edge stretch performance with an adequate sample size; however, challenges exist for use for lot acceptance testing.



Hole Expansion Test

? Mechanical properties of select grades for hole expansion testing.

? Current production DP780 and DP980 vs. newer RA-bearing 1180 MPa grades.

? Mechanical properties of select grades for hole expansion testing.

? Current production DP780 and DP980 vs. newer RA-bearing 1180 MPa grades.


? Newer high strength 1180 MPa grades showing >= HER vs. more conventional DP steels and less sensitivity to edge condition.

? New grades need balance of global and local formability for most applications.

Nano-Indentation Evaluation – DP780

? Nano-indentation testing was performed to determine constituent hardness distributions in mixed microstructure DP780 steel.

? Two production samples were acquired representing two steel sources.

? Under similar blanking and stamping conditions, one steel exhibited edge fracture while the other did not.

? Samples were ground/polished using standard metallurgical techniques and finish-polished with colloidal silica.


? MTS Nanoindenter XP was used.

? Testing was performed at room emperature with a Berkovich tip

? Displacement control was used to indent to 100 nm maximum depth

? 12 x 12 array of indents was placed on each specimen, spaced

2 μm apart ? Resulting hardness was averaged over a 60-90 nm depth to remove any surface abnormalities


Summary

? Edge fracture susceptibility is influenced by a variety of related factors: blank edge condition, material, part design / forming (strain distribution) / trimming process.

? A balance of global and local formability performance is required for most cold-stamped parts and shall be considered in steel development.

? Uniform, fine-grained structure required

? Reduced hardness differential between constituents

? An industry-wide test is needed for material lot acceptance to predict edge fracture susceptibility

? Performance not predicted by standard tensile testing.





Write a Comment
Ten multiply Two =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 日本亚洲欧美高清专区vr专区| 青青草原亚洲| 韩国三级丰满少妇高潮| 国产一精品一av一免费爽爽| 韩国三级在线 中文字幕 无码| 国产精品户露av在线户外直播| 无码一区二区三区不卡av| 亚洲三区在线观看无套内射| 成 人 免费观看网站| 亚洲人成网站在线观看播放 | 无码熟妇人妻av在线影片最多| 国产在线高清理伦片a| 亚洲国产一区二区精品无码| 成人午夜福利免费体验区| a在线视频v视频| 日日摸日日碰夜夜爽亚洲| 免费看无码特级毛片| 国产超碰无码最新上传| 一本一本久久a久久综合精品| 色播久久人人爽人人爽人人片av| 日韩免费无码视频一区二区三区| 天堂中文最新版在线中文| 精品国产男人的天堂久久| 欧美熟妇性xxxx欧美熟人多毛| 精品传媒一区二区| 99久久精品国产一区二区蜜芽| 欧美成人一区二区三区在线视频| 亚洲日本精品麻豆一区国产| 一区二区三区在线观看国产精品 | 欧美尺码专线欧洲b1b1| 天干夜天干天天天爽视频| 亚洲精品国产精品国产自| 国产综合视频一区二区三区| 国产免费艾彩sm调教视频| 日韩精品中文字幕无码一区| 91久久久人妻精品国产一区二区| 亚洲一卡二卡三卡四卡| 国产欧美国产综合每日更新| 337p粉嫩日本欧洲亚洲大胆| 3344永久在线观看视频| 亚洲国产精品成人久久蜜臀 |